The testing rate for the samples were 5 mm/min (83 um/sec).
Wednesday, September 26, 2012
Adhesion Results
This is a plot of 5-1 PDMS-1k Plain weave carbon fiber graph. There seems to be improved adhesion in all of the patterns, the larger increase in the orthogonally patterned samples than the parallel ones.
Tuesday, September 25, 2012
Suppression of Fracture
In this posting, I am comparing the shear testing of a non-patterned 5-1 PDMS/Plain Weave 1k Carbon Fiber composite with that of a patterned surface. The magnification of these features are 2.5 x and the pulling velocity of the tests are 83 micrometers/sec (5 mm/min). All of the samples are being pulled from the left side.
This is the sample immediately before the fracture.
Sample after fracture occurs (time elapsed between the two samples ~150 msec)
This is the sample immediately before the fracture.
Sample after fracture occurs (time elapsed between the two samples ~150 msec)
Fracture occurs rapidly and typically the fracture across the interface occurs faster than the rate of data acquisition for the adhesion program. However, when the samples are patterned such as the orthogonal one below:
The first picture is of the orthogonal CD pattern in the loading part of the curve. The second picture is that of the same pattern at the critical force. After the critical force is reached, the sample begins to slide and there is no precipitous drop in force. As the sample drags, fractures coalesce, however contact area can be reformed as well, shown below:
The sample as in the other images is being pulled from the left side. The fractures move to the right and contact area becomes reestablished on the left side of the sample when the sample is sliding. The brightest regions are where there is a fracture. The slightly darker regions are those where the top of the patterns are in contact but not the bottoms. The darkest are where the features are completely compressed and in contact with the substrate. The squares are the gaps in the weave structure.
Parallel patterns behave the same way, in this case the lines are parallel to the pull direction, so the fracture initiate faster in the perpendicular direction than the orthogonal patterns.
Tuesday, July 3, 2012
Stress Relaxation
Here is a stress relaxation curve for a PDMS sample I have prepared. The approach speed is 100 um/sec and the dwell time is 300 sec. The data points on the curve are from the force displacement and then divided by the corresponding area that I measured in image J. The fit on the curve is shown below:
Wednesday, June 27, 2012
Adhesion of partially cured PDMS
I have attached a couple of force vs displacement curves for a measured partially cured PDMS sample and the predicted force displacement curve, taking into account the confinement in the sample, since a typical a/h value is 0.1-0.8 for these tests. This particular plot is for the partially cured PDMS sample was ran at 50 um/sec. It should be noted, this was not the first run on this particular PDMS, the first test run on this sample (in a different location on the sample) was 100 um/sec. So just to keep in mind that this would correspond to a longer processing time (2 minutes or so, opposed to 30 seconds). The small curve in between the linear lines is the loading cycle and the two divergent linear lines are the unloading cycles.
The ring on the perimeter will change size depending on the stage of the unloading, however becomes large at the very end. There is also a loss of circularity towards the end as well. This was observed in the first test at 100 um/sec as well, where there was a non-circular contact area at the end of unloading. In both the 100 um/sec and 50 um/sec samples, there was also some necking that occurred.
The plots appear to begin to diverge on the unloading cycle and they are convergent on the compression loading of the cycle. Below is an image of the sample being unloaded in the 50 um/sec sample to show a concentric ring, which appears to possibly be cavitation.
Sunday, June 24, 2012
SEM Cross-sections
The images shown are representative of a cross-section area we took with the fibers embedded in PDMS. In order to image this, we made a PDMS substrate with carbon fibers and then collected a 500 nm colloidal array on top. Next, that sample was turned 90 and embedded in more PDMS. Afterwards, the "composite" of the substrate embedded with PDMS was cut for a cross-section area. This was done to hold the fibers in place and not allow them to move. When we cut the samples for a cross section with no embedding, the fibers would move out of the substrate. Alternatively, when we repeated this embedding in epoxy, there were adhesion problems and the fibers would transfer to the epoxy. Below are three images of the same fiber from several angles.
The problem with this method of embedding in PDMS is that the PDMS creates better adhesion to the colloids than the carbon fiber and thus they are stripped off the surface. However, we have not be able to get the cross section on the PDMS substrate without embedding. Unlike the fabrics, the individual fibers do not remain still when the cutting occurs.
The problem with this method of embedding in PDMS is that the PDMS creates better adhesion to the colloids than the carbon fiber and thus they are stripped off the surface. However, we have not be able to get the cross section on the PDMS substrate without embedding. Unlike the fabrics, the individual fibers do not remain still when the cutting occurs.
Monday, May 28, 2012
Angle Dependence on Colloidal Coating
No pictures for the first part of the blog posting, so I will sum up the latest observations I have made on the colloidal coating on various substrates :
For reference, when I say degrees, I am talking about the angle of the substrate with the surface of the water (or film, 0 = parallel, 90 = perpendicular), these were also drawn by hand.
-Glass and UVO treated silicon coat very well at three angles, I have tested 0, 45 and 90 degrees (using a protactor and setting the angle) for these samples. However, one drawback to this is if there are high amounts of fibers around, they can aggregate when the fiber is drawn, this is likely due to the fact there is poor adhesion between the glass and the carbon fiber.
-Untreated PDMS works best at angles below 15 degrees, because of the hydrophobicity, the water underneath the film slides very easily at higher angles.
-Treating PDMS and Fibers with UVO for short times (5 min) helps, but does not do considerable amount of difference.
The bottom is a picture of 500 nm colloid coated carbon fiber from a copper grid substrate again, taken today:
Copper grid appears to work just as well as the PDMS substrate in terms of the coating (on the supported part, this part of the fiber is not free standing).
For reference, when I say degrees, I am talking about the angle of the substrate with the surface of the water (or film, 0 = parallel, 90 = perpendicular), these were also drawn by hand.
-Glass and UVO treated silicon coat very well at three angles, I have tested 0, 45 and 90 degrees (using a protactor and setting the angle) for these samples. However, one drawback to this is if there are high amounts of fibers around, they can aggregate when the fiber is drawn, this is likely due to the fact there is poor adhesion between the glass and the carbon fiber.
-Untreated PDMS works best at angles below 15 degrees, because of the hydrophobicity, the water underneath the film slides very easily at higher angles.
-Treating PDMS and Fibers with UVO for short times (5 min) helps, but does not do considerable amount of difference.
The bottom is a picture of 500 nm colloid coated carbon fiber from a copper grid substrate again, taken today:
Copper grid appears to work just as well as the PDMS substrate in terms of the coating (on the supported part, this part of the fiber is not free standing).
Thursday, May 24, 2012
Colloidal Coating 2
Colloidal Coating Part 1
In this post there are several pictures of colloidal films being draped over carbon fiber in different configurations with different results:
In these two in the top, a 500 nm PS colloidal film was draped over an array of carbon fibers supported on a copper mesh. These particular components of the fibers were supporeted by the copper meshing itself (not freestanding). The copper meshing and the carbon fiber are coated very well as seen when the fiber is supported on PDMS.
In the next two pictures, these carbon fibers were freestanding over the copper meshing (span length = 1mm, maximum). The particles have good ordering, except for the large protrusions off the fiber. The film breaks into several films around the fiber.
In the final two pictures for this section, this was 500 nm particles were the fibers were again free standing, but the span length was 2.5 cm long. These are taken from the "bottom" relative to the withdrawing direction. Although these two are coated well, the coating of the fibers very inconsistent. Furthermore, if there is a higher density of fibers, they will collapse due to capillary forces. In the next post, I will show a couple of structures with patterned and unpatterned areas.
In these two in the top, a 500 nm PS colloidal film was draped over an array of carbon fibers supported on a copper mesh. These particular components of the fibers were supporeted by the copper meshing itself (not freestanding). The copper meshing and the carbon fiber are coated very well as seen when the fiber is supported on PDMS.
In the next two pictures, these carbon fibers were freestanding over the copper meshing (span length = 1mm, maximum). The particles have good ordering, except for the large protrusions off the fiber. The film breaks into several films around the fiber.
In the final two pictures for this section, this was 500 nm particles were the fibers were again free standing, but the span length was 2.5 cm long. These are taken from the "bottom" relative to the withdrawing direction. Although these two are coated well, the coating of the fibers very inconsistent. Furthermore, if there is a higher density of fibers, they will collapse due to capillary forces. In the next post, I will show a couple of structures with patterned and unpatterned areas.
Friday, May 18, 2012
Adhesion with CF-F-15 with laminated tendon
In this blog post, this is a follow up from the last posting. I tested the DVD and CD patterns on both smooth glass and frosted glass to test the adhesion. The orthogonal arrangement produced the highest adhesion in both the DVD and CD pattern on smooth glass (42% and 50% better respectively than the non-patterned). Parallel both did better than the non-patterned substrate (16% for CD and 22% for DVD), but not as great as the orthogonal. However, on the rough surface of frosted glass, only the DVD-Orthogonal performed better, and even so, not a significant difference. The DVD appears to perform better than the CD features regardless of configuration.
Wednesday, May 9, 2012
Contact of the Lines
In these pictures, we first show a picture of a glass slide. Next, a PDMS patterned CD pattern was placed on and watched as it established contact with the surface. Finally, when the PDMS has more force applied, the contact becomes even more intimate to the surface. In the second picture, the darker side is in contact with the surface and the surface continues to bring itself into contact with the glass. In the first contact phase, the diffraction patterns are still apparent, although they are diminished slightly. As the structures, move into the darkest region, the diffraction pattern is no longer visible, indicating the structure has collapsed.
In all three pictures, the lines are relatively running up and down. When the contact is established during the collapse of the structures, the contact propagates parallel to the lines.
Adhesion of Carbon Fiber-F-15 Samples on Smooth Glass
In these samples, I kept the dimensions of the samples equivalent from the previously mentioned samples, however this time I put resin on the entire tendon, rather than just the patterned area. This was done in order to keep the stress distribution along the fabric more constant that previous tests. In this case, the orthogonal sample provided the highest adhesion, 50% more than an unpatterned substrate. The parallel case had an adhesion increase of about 15%.
Thursday, April 26, 2012
Patterned Adhesion-2
Here are more plots of patterned adhesion that were performed with a Nylon backing and F-15 polyurethane. F-15 is a very nice polyurethane for replicating features. Once again, the parallel orientation of the features produces the highest improvement on the adhesion, regardless of the pitch size. In order to eliminate variables, the samples produced were ~ 4 cm^2 in the patterned region (ca. 2 x 2 cm), with the exception of the orthogonal CD pattern, which was smaller in the width, due to defects in the sample. However, in that case, the area remained comparable to the other samples, by keeping the length longer.
Tuesday, April 24, 2012
Patterned adhesion photos
In this photo, there are the 5 samples that were tested in the last post. From left to right: Non-patterned, CD-Orthogonal, CD-Parallel, DVD-Orthogonal, DVD-Parallel. In all of the samples, the distance between the top of the clamping and the bottom of the patterned feature is 4 cm, this is held constant in all of the samples, as well as the other previously tested samples. All of the samples were produced from a 4 cm wide and 10 cm long piece of 1k 2-D carbon fiber. The patterned area typically ranges from 7-10 cm^2, depending on the type of mold and if defects were present on the edges of the sample that were removed. The size discrepancy of the molds, particularly between orthogonal and parallel samples arises from limitations of the CD or DVD disk size in the radial direction. The edges are trimmed off in order to eliminate edge effects that arise when resin wicks over the mold. The bottom of the samples are not this messy or frayed when they are tested, this is a result of pulling the fabric off of a layer of scotch tape that is used to hold the sample down in the clamp.
Monday, April 23, 2012
Patterned Adhesion with Composites
In these experiments, 5 composites were made with 2-D (orthotropic) carbon fibers (1k) and F-15 polyurethane resin. One sample was left unpatterned as a control sample to compare how features effect adhesion. Two samples were created with a CD pattern, one with the lines running parallel to the straining direction and one orthogonal to the straining direction. This was also repeated with a DVD pattern to compare two different size pitches. The adhesion results are posted below with the adhesion in N/cm2 and the second graph is the normalized adhesion compared to the unpatterned surface. All of these samples were tested for their adhesion on three different surfaces: Smooth glass, Frosted Glass and Painted Steel to evaluate the effect of different surface roughness on the adhesion.
The patterns with the CD features appear to do better than smooth samples in all three surfaces. DVD patterns did better in the smooth adhesion, but not in the roughness. One possibility is that since these features are smaller than the roughness, it may have a hard time fitting in and thus compromising the ability to adhere. In the CD the patterns are closer to the size of the roughness, and thus may be able to accommodate roughness better in the trenches. More tests will follow on other substrates, it took a few attempts to get a fairly consistent replicating method.
Thursday, April 21, 2011
Caviation with Artificial Appendages
In the sequence below, you can see an appendage from the Mantis Shrimp molded from Norland Optical 60, creates cavitation in water as it moves. The first image on the left is the appendage at the initial rest position, the center one is a position where cavitation is beginning to form and then the final image is a larger cavity formed. One interesting thing to note is that the appendage slows down considerably after cavitation. This cavitation effect is also observed in samples made from 2-P and both materials survive the testing process without breaking.
We (Suzanne and I) have about 24 new samples to test with 5 different sizes made from both materials (2-P only in some cases), and 3 samples of each to gather statistics within each sample and to observe possible roughness effects from the mold.


We (Suzanne and I) have about 24 new samples to test with 5 different sizes made from both materials (2-P only in some cases), and 3 samples of each to gather statistics within each sample and to observe possible roughness effects from the mold.


Monday, March 28, 2011
Dry CO2 exposure in Glovebag and Adhesion

Here is a force vs. displacement curve for two glass surfaces treated with a 21 hour vapor exposure of N-(2-ethylamino)-3-aminopropyl trimethoxysilane. One of the surfaces was left untreated, the second one was left in a glove bag for 2 hours under a dry N2 gas purge. Following the purge, the sample was exposed to a 90 second exposure to "Bone Dry" Grade CO2 in the same glove bag. The sample exposed to CO2 showed very little change in contact angle measurements. Here is the force vs. displacement curve for the two samples and little differences were exhibited in the adhesion.
Monday, January 31, 2011
Submerged Adhesion of Amino Functionalize Surfaces
In this picture, this is a force vs. displacement for a PDMS probe on non-functionalized glass (red), amine functionalized glass (N-ethylamino-3proplyaminetrimethoxysilane, in blue), and the same silane treatement with CO2 exposure (in green). The probe speed was 1 micron/sec. Subsequent trials of this adhesion test will follow shortly.
Wednesday, December 8, 2010
Compression Testing of Amine Layers
In this sequence of microscope images (2.5 x magnification), a glass probe was compressed against glass slide samples that were prepared on 10-12-2010 with N-(2-aminoethyl)-3-aminopropyl-trimethoxysilane as the layer. The top image is that of the probe coming into contact with a large droplet and compressing down to 1 g of force on a glass slide that has had CO2 added to it. The second droplet is another image of the same slide, however this time the compression test was done on an area that did not have a large droplet. The third image is that of the same silane treatment, but a sample that has not had any CO2 added at all. The scale bar for all three images is 500 microns and all of these images are at the point of maximum force applied.




Monday, October 18, 2010
Drying Effects
More on the contact angles will be posted when I compile a couple of more samples, but for now here are some images of the effects of drying the samples with CO2 gas versus air when wet with water. The samples were prepared by vapor deposition, similar to the procedure used in prior blog postings. The pictures are: Amine surface [N-(2-aminoethyl)-3-aminopropyl-trimethoxysilane] after drying with CO2 (top left), air dry (bottom left), formamidine functionalized with CO2 drying (top right) and formamidine functionalized with air drying (bottom right). The magnification of these pictures is 5x ( I apologize for no scale bars).






Thursday, October 7, 2010
More contact angle measurements
Continuing from the last post, here are the contact angles of the converted amine surfaces to amidine surfaces:
With CO2 in water treatment for 5 minutes:
75.4 +/- 2.9 (Advancing)
32.0 +/- 3.4 (Receding)
With N2 in water treatment for 5 minutes:
80.6 +/- 2.2 (Advancing)
29.6 +/- 6.4 (Receding)
With CO2 in water treatment for 5 minutes:
75.4 +/- 2.9 (Advancing)
32.0 +/- 3.4 (Receding)
With N2 in water treatment for 5 minutes:
80.6 +/- 2.2 (Advancing)
29.6 +/- 6.4 (Receding)