Monday, May 28, 2012

Angle Dependence on Colloidal Coating

No pictures for the first part of the blog posting, so I will sum up the latest observations I have made on the colloidal coating on various substrates :

For reference, when I say degrees, I am talking about the angle of the substrate with the surface of the water (or film, 0 = parallel, 90 = perpendicular), these were also drawn by hand.

-Glass and UVO treated silicon coat very well at three angles,  I have tested 0, 45 and 90 degrees (using a protactor and setting the angle) for these samples.  However, one drawback to this is if there are high amounts of fibers around, they can aggregate when the fiber is drawn, this is likely due to the fact there is poor adhesion between the glass and the carbon fiber.

-Untreated PDMS works best at angles below 15 degrees, because of the hydrophobicity, the water underneath the film slides very easily at higher angles.

-Treating PDMS and Fibers with UVO for short times (5 min) helps, but does not do considerable amount of difference.

The bottom is a picture of 500 nm colloid coated carbon fiber from a copper grid substrate again, taken today:

Copper grid appears to work just as well as the PDMS substrate in terms of the coating (on the supported part, this part of the fiber is not free standing).

Thursday, May 24, 2012

Colloidal Coating 2



In these two pictures above the 500 nm PS colloids are residing on the part of the fibers that were draped.  The second figure is tilted 50 degrees and is on the edge of the copper interface, meaning to the right of the fiber, the fiber is supported. 

The final picture is the bottom side (relative to the collecting direction of the film) of carbon fibers residing on a copper meshing.  To the left, right and the other side of the fiber are 200 nm PS colloids and SDS surfactant.  The center of the picture is uncovered carbon fiber, where the film was unable to wrap around the fiber, leave an exposed or "Janus" structure.  Will take the "top side" on next available SEM time.  

Colloidal Coating Part 1

In this post there are several pictures of colloidal films being draped over carbon fiber in different configurations with different results:


In these two in the top, a 500 nm PS colloidal film was draped over an array of carbon fibers supported on a copper mesh.  These particular components of the fibers were supporeted by the copper meshing itself (not freestanding).  The copper meshing and the carbon fiber are coated very well as seen when the fiber is supported on PDMS.


In the next two pictures, these carbon fibers were freestanding over the copper meshing (span length = 1mm, maximum).  The particles have good ordering, except for the large protrusions off the fiber.  The film breaks into several films around the fiber.

In the final two pictures for this section, this was 500 nm particles were the fibers were again free standing, but the span length was 2.5 cm long.  These are taken from the "bottom" relative to the withdrawing direction.  Although these two are coated well, the coating of the fibers very inconsistent.  Furthermore, if there is a higher density of fibers, they will collapse due to capillary forces.  In the next post, I will show a couple of structures with patterned and unpatterned areas.

Friday, May 18, 2012

Adhesion with CF-F-15 with laminated tendon

In this blog post, this is a follow up from the last posting.  I tested the DVD and CD patterns on both smooth glass and frosted glass to test the adhesion.  The orthogonal arrangement produced the highest adhesion in both the DVD and CD pattern on smooth glass (42% and 50% better respectively than the non-patterned).  Parallel both did better than the non-patterned substrate (16% for CD and 22% for DVD), but not as great as the orthogonal.  However, on the rough surface of frosted glass, only the DVD-Orthogonal performed better, and even so, not a significant difference.  The DVD appears to perform better than the CD features regardless of configuration.

Wednesday, May 9, 2012

Contact of the Lines



In these pictures, we first show a picture of a glass slide.  Next, a PDMS patterned CD pattern was placed on and watched as it established contact with the surface.  Finally, when the PDMS has more force applied, the contact becomes even more intimate to the surface.  In the second picture, the darker side is in contact with the surface and the surface continues to bring itself into contact with the glass.  In the first contact phase, the diffraction patterns are still apparent, although they are diminished slightly.  As the structures, move into the darkest region, the diffraction pattern is no longer visible, indicating the structure has collapsed.

In all three pictures, the lines are relatively running up and down.  When the contact is established during the collapse of the structures, the contact propagates parallel to the lines.

Adhesion of Carbon Fiber-F-15 Samples on Smooth Glass

In these samples, I kept the dimensions of the samples equivalent from the previously mentioned samples, however this time I put resin on the entire tendon, rather than just the patterned area.  This was done in order to keep the stress distribution along the fabric more constant that previous tests.  In this case, the orthogonal sample provided the highest adhesion, 50% more than an unpatterned substrate.  The parallel case had an adhesion increase of about 15%.