Here are more plots of patterned adhesion that were performed with a Nylon backing and F-15 polyurethane. F-15 is a very nice polyurethane for replicating features. Once again, the parallel orientation of the features produces the highest improvement on the adhesion, regardless of the pitch size. In order to eliminate variables, the samples produced were ~ 4 cm^2 in the patterned region (ca. 2 x 2 cm), with the exception of the orthogonal CD pattern, which was smaller in the width, due to defects in the sample. However, in that case, the area remained comparable to the other samples, by keeping the length longer.
Thursday, April 26, 2012
Tuesday, April 24, 2012
Patterned adhesion photos
In this photo, there are the 5 samples that were tested in the last post. From left to right: Non-patterned, CD-Orthogonal, CD-Parallel, DVD-Orthogonal, DVD-Parallel. In all of the samples, the distance between the top of the clamping and the bottom of the patterned feature is 4 cm, this is held constant in all of the samples, as well as the other previously tested samples. All of the samples were produced from a 4 cm wide and 10 cm long piece of 1k 2-D carbon fiber. The patterned area typically ranges from 7-10 cm^2, depending on the type of mold and if defects were present on the edges of the sample that were removed. The size discrepancy of the molds, particularly between orthogonal and parallel samples arises from limitations of the CD or DVD disk size in the radial direction. The edges are trimmed off in order to eliminate edge effects that arise when resin wicks over the mold. The bottom of the samples are not this messy or frayed when they are tested, this is a result of pulling the fabric off of a layer of scotch tape that is used to hold the sample down in the clamp.
Monday, April 23, 2012
Patterned Adhesion with Composites
In these experiments, 5 composites were made with 2-D (orthotropic) carbon fibers (1k) and F-15 polyurethane resin. One sample was left unpatterned as a control sample to compare how features effect adhesion. Two samples were created with a CD pattern, one with the lines running parallel to the straining direction and one orthogonal to the straining direction. This was also repeated with a DVD pattern to compare two different size pitches. The adhesion results are posted below with the adhesion in N/cm2 and the second graph is the normalized adhesion compared to the unpatterned surface. All of these samples were tested for their adhesion on three different surfaces: Smooth glass, Frosted Glass and Painted Steel to evaluate the effect of different surface roughness on the adhesion.
The patterns with the CD features appear to do better than smooth samples in all three surfaces. DVD patterns did better in the smooth adhesion, but not in the roughness. One possibility is that since these features are smaller than the roughness, it may have a hard time fitting in and thus compromising the ability to adhere. In the CD the patterns are closer to the size of the roughness, and thus may be able to accommodate roughness better in the trenches. More tests will follow on other substrates, it took a few attempts to get a fairly consistent replicating method.
Thursday, April 21, 2011
Caviation with Artificial Appendages
In the sequence below, you can see an appendage from the Mantis Shrimp molded from Norland Optical 60, creates cavitation in water as it moves. The first image on the left is the appendage at the initial rest position, the center one is a position where cavitation is beginning to form and then the final image is a larger cavity formed. One interesting thing to note is that the appendage slows down considerably after cavitation. This cavitation effect is also observed in samples made from 2-P and both materials survive the testing process without breaking.
We (Suzanne and I) have about 24 new samples to test with 5 different sizes made from both materials (2-P only in some cases), and 3 samples of each to gather statistics within each sample and to observe possible roughness effects from the mold.


We (Suzanne and I) have about 24 new samples to test with 5 different sizes made from both materials (2-P only in some cases), and 3 samples of each to gather statistics within each sample and to observe possible roughness effects from the mold.


Monday, March 28, 2011
Dry CO2 exposure in Glovebag and Adhesion

Here is a force vs. displacement curve for two glass surfaces treated with a 21 hour vapor exposure of N-(2-ethylamino)-3-aminopropyl trimethoxysilane. One of the surfaces was left untreated, the second one was left in a glove bag for 2 hours under a dry N2 gas purge. Following the purge, the sample was exposed to a 90 second exposure to "Bone Dry" Grade CO2 in the same glove bag. The sample exposed to CO2 showed very little change in contact angle measurements. Here is the force vs. displacement curve for the two samples and little differences were exhibited in the adhesion.
Monday, January 31, 2011
Submerged Adhesion of Amino Functionalize Surfaces
In this picture, this is a force vs. displacement for a PDMS probe on non-functionalized glass (red), amine functionalized glass (N-ethylamino-3proplyaminetrimethoxysilane, in blue), and the same silane treatement with CO2 exposure (in green). The probe speed was 1 micron/sec. Subsequent trials of this adhesion test will follow shortly.
Wednesday, December 8, 2010
Compression Testing of Amine Layers
In this sequence of microscope images (2.5 x magnification), a glass probe was compressed against glass slide samples that were prepared on 10-12-2010 with N-(2-aminoethyl)-3-aminopropyl-trimethoxysilane as the layer. The top image is that of the probe coming into contact with a large droplet and compressing down to 1 g of force on a glass slide that has had CO2 added to it. The second droplet is another image of the same slide, however this time the compression test was done on an area that did not have a large droplet. The third image is that of the same silane treatment, but a sample that has not had any CO2 added at all. The scale bar for all three images is 500 microns and all of these images are at the point of maximum force applied.