Tuesday, July 3, 2012
Stress Relaxation
Here is a stress relaxation curve for a PDMS sample I have prepared. The approach speed is 100 um/sec and the dwell time is 300 sec. The data points on the curve are from the force displacement and then divided by the corresponding area that I measured in image J. The fit on the curve is shown below:
Wednesday, June 27, 2012
Adhesion of partially cured PDMS
I have attached a couple of force vs displacement curves for a measured partially cured PDMS sample and the predicted force displacement curve, taking into account the confinement in the sample, since a typical a/h value is 0.1-0.8 for these tests. This particular plot is for the partially cured PDMS sample was ran at 50 um/sec. It should be noted, this was not the first run on this particular PDMS, the first test run on this sample (in a different location on the sample) was 100 um/sec. So just to keep in mind that this would correspond to a longer processing time (2 minutes or so, opposed to 30 seconds). The small curve in between the linear lines is the loading cycle and the two divergent linear lines are the unloading cycles.
The ring on the perimeter will change size depending on the stage of the unloading, however becomes large at the very end. There is also a loss of circularity towards the end as well. This was observed in the first test at 100 um/sec as well, where there was a non-circular contact area at the end of unloading. In both the 100 um/sec and 50 um/sec samples, there was also some necking that occurred.
The plots appear to begin to diverge on the unloading cycle and they are convergent on the compression loading of the cycle. Below is an image of the sample being unloaded in the 50 um/sec sample to show a concentric ring, which appears to possibly be cavitation.
Sunday, June 24, 2012
SEM Cross-sections
The images shown are representative of a cross-section area we took with the fibers embedded in PDMS. In order to image this, we made a PDMS substrate with carbon fibers and then collected a 500 nm colloidal array on top. Next, that sample was turned 90 and embedded in more PDMS. Afterwards, the "composite" of the substrate embedded with PDMS was cut for a cross-section area. This was done to hold the fibers in place and not allow them to move. When we cut the samples for a cross section with no embedding, the fibers would move out of the substrate. Alternatively, when we repeated this embedding in epoxy, there were adhesion problems and the fibers would transfer to the epoxy. Below are three images of the same fiber from several angles.
The problem with this method of embedding in PDMS is that the PDMS creates better adhesion to the colloids than the carbon fiber and thus they are stripped off the surface. However, we have not be able to get the cross section on the PDMS substrate without embedding. Unlike the fabrics, the individual fibers do not remain still when the cutting occurs.
The problem with this method of embedding in PDMS is that the PDMS creates better adhesion to the colloids than the carbon fiber and thus they are stripped off the surface. However, we have not be able to get the cross section on the PDMS substrate without embedding. Unlike the fabrics, the individual fibers do not remain still when the cutting occurs.
Monday, May 28, 2012
Angle Dependence on Colloidal Coating
No pictures for the first part of the blog posting, so I will sum up the latest observations I have made on the colloidal coating on various substrates :
For reference, when I say degrees, I am talking about the angle of the substrate with the surface of the water (or film, 0 = parallel, 90 = perpendicular), these were also drawn by hand.
-Glass and UVO treated silicon coat very well at three angles, I have tested 0, 45 and 90 degrees (using a protactor and setting the angle) for these samples. However, one drawback to this is if there are high amounts of fibers around, they can aggregate when the fiber is drawn, this is likely due to the fact there is poor adhesion between the glass and the carbon fiber.
-Untreated PDMS works best at angles below 15 degrees, because of the hydrophobicity, the water underneath the film slides very easily at higher angles.
-Treating PDMS and Fibers with UVO for short times (5 min) helps, but does not do considerable amount of difference.
The bottom is a picture of 500 nm colloid coated carbon fiber from a copper grid substrate again, taken today:
Copper grid appears to work just as well as the PDMS substrate in terms of the coating (on the supported part, this part of the fiber is not free standing).
For reference, when I say degrees, I am talking about the angle of the substrate with the surface of the water (or film, 0 = parallel, 90 = perpendicular), these were also drawn by hand.
-Glass and UVO treated silicon coat very well at three angles, I have tested 0, 45 and 90 degrees (using a protactor and setting the angle) for these samples. However, one drawback to this is if there are high amounts of fibers around, they can aggregate when the fiber is drawn, this is likely due to the fact there is poor adhesion between the glass and the carbon fiber.
-Untreated PDMS works best at angles below 15 degrees, because of the hydrophobicity, the water underneath the film slides very easily at higher angles.
-Treating PDMS and Fibers with UVO for short times (5 min) helps, but does not do considerable amount of difference.
The bottom is a picture of 500 nm colloid coated carbon fiber from a copper grid substrate again, taken today:
Copper grid appears to work just as well as the PDMS substrate in terms of the coating (on the supported part, this part of the fiber is not free standing).
Thursday, May 24, 2012
Colloidal Coating 2
Colloidal Coating Part 1
In this post there are several pictures of colloidal films being draped over carbon fiber in different configurations with different results:
In these two in the top, a 500 nm PS colloidal film was draped over an array of carbon fibers supported on a copper mesh. These particular components of the fibers were supporeted by the copper meshing itself (not freestanding). The copper meshing and the carbon fiber are coated very well as seen when the fiber is supported on PDMS.
In the next two pictures, these carbon fibers were freestanding over the copper meshing (span length = 1mm, maximum). The particles have good ordering, except for the large protrusions off the fiber. The film breaks into several films around the fiber.
In the final two pictures for this section, this was 500 nm particles were the fibers were again free standing, but the span length was 2.5 cm long. These are taken from the "bottom" relative to the withdrawing direction. Although these two are coated well, the coating of the fibers very inconsistent. Furthermore, if there is a higher density of fibers, they will collapse due to capillary forces. In the next post, I will show a couple of structures with patterned and unpatterned areas.
In these two in the top, a 500 nm PS colloidal film was draped over an array of carbon fibers supported on a copper mesh. These particular components of the fibers were supporeted by the copper meshing itself (not freestanding). The copper meshing and the carbon fiber are coated very well as seen when the fiber is supported on PDMS.
In the next two pictures, these carbon fibers were freestanding over the copper meshing (span length = 1mm, maximum). The particles have good ordering, except for the large protrusions off the fiber. The film breaks into several films around the fiber.
In the final two pictures for this section, this was 500 nm particles were the fibers were again free standing, but the span length was 2.5 cm long. These are taken from the "bottom" relative to the withdrawing direction. Although these two are coated well, the coating of the fibers very inconsistent. Furthermore, if there is a higher density of fibers, they will collapse due to capillary forces. In the next post, I will show a couple of structures with patterned and unpatterned areas.
Friday, May 18, 2012
Adhesion with CF-F-15 with laminated tendon
In this blog post, this is a follow up from the last posting. I tested the DVD and CD patterns on both smooth glass and frosted glass to test the adhesion. The orthogonal arrangement produced the highest adhesion in both the DVD and CD pattern on smooth glass (42% and 50% better respectively than the non-patterned). Parallel both did better than the non-patterned substrate (16% for CD and 22% for DVD), but not as great as the orthogonal. However, on the rough surface of frosted glass, only the DVD-Orthogonal performed better, and even so, not a significant difference. The DVD appears to perform better than the CD features regardless of configuration.