Thursday, May 24, 2012

Colloidal Coating Part 1

In this post there are several pictures of colloidal films being draped over carbon fiber in different configurations with different results:


In these two in the top, a 500 nm PS colloidal film was draped over an array of carbon fibers supported on a copper mesh.  These particular components of the fibers were supporeted by the copper meshing itself (not freestanding).  The copper meshing and the carbon fiber are coated very well as seen when the fiber is supported on PDMS.


In the next two pictures, these carbon fibers were freestanding over the copper meshing (span length = 1mm, maximum).  The particles have good ordering, except for the large protrusions off the fiber.  The film breaks into several films around the fiber.

In the final two pictures for this section, this was 500 nm particles were the fibers were again free standing, but the span length was 2.5 cm long.  These are taken from the "bottom" relative to the withdrawing direction.  Although these two are coated well, the coating of the fibers very inconsistent.  Furthermore, if there is a higher density of fibers, they will collapse due to capillary forces.  In the next post, I will show a couple of structures with patterned and unpatterned areas.

Friday, May 18, 2012

Adhesion with CF-F-15 with laminated tendon

In this blog post, this is a follow up from the last posting.  I tested the DVD and CD patterns on both smooth glass and frosted glass to test the adhesion.  The orthogonal arrangement produced the highest adhesion in both the DVD and CD pattern on smooth glass (42% and 50% better respectively than the non-patterned).  Parallel both did better than the non-patterned substrate (16% for CD and 22% for DVD), but not as great as the orthogonal.  However, on the rough surface of frosted glass, only the DVD-Orthogonal performed better, and even so, not a significant difference.  The DVD appears to perform better than the CD features regardless of configuration.

Wednesday, May 9, 2012

Contact of the Lines



In these pictures, we first show a picture of a glass slide.  Next, a PDMS patterned CD pattern was placed on and watched as it established contact with the surface.  Finally, when the PDMS has more force applied, the contact becomes even more intimate to the surface.  In the second picture, the darker side is in contact with the surface and the surface continues to bring itself into contact with the glass.  In the first contact phase, the diffraction patterns are still apparent, although they are diminished slightly.  As the structures, move into the darkest region, the diffraction pattern is no longer visible, indicating the structure has collapsed.

In all three pictures, the lines are relatively running up and down.  When the contact is established during the collapse of the structures, the contact propagates parallel to the lines.

Adhesion of Carbon Fiber-F-15 Samples on Smooth Glass

In these samples, I kept the dimensions of the samples equivalent from the previously mentioned samples, however this time I put resin on the entire tendon, rather than just the patterned area.  This was done in order to keep the stress distribution along the fabric more constant that previous tests.  In this case, the orthogonal sample provided the highest adhesion, 50% more than an unpatterned substrate.  The parallel case had an adhesion increase of about 15%.


Thursday, April 26, 2012

Patterned Adhesion-2

Here are more plots of patterned adhesion that were performed with a Nylon backing and F-15 polyurethane.  F-15 is a very nice polyurethane for replicating features.  Once again, the parallel orientation of the features produces the highest improvement on the adhesion, regardless of the pitch size.  In order to eliminate variables, the samples produced were ~ 4 cm^2 in the patterned region (ca. 2 x 2 cm), with the exception of the orthogonal CD pattern, which was smaller in the width, due to defects in the sample.  However, in that case, the area remained comparable to the other samples, by keeping the length longer.



Tuesday, April 24, 2012

Patterned adhesion photos

In this photo, there are the 5 samples that were tested in the last post.  From left to right: Non-patterned, CD-Orthogonal, CD-Parallel, DVD-Orthogonal, DVD-Parallel.  In all of the samples, the distance between the top of the clamping and the bottom of the patterned feature is 4 cm, this is held constant in all of the samples, as well as the other previously tested samples.  All of the samples were produced from a 4 cm wide and 10 cm long piece of 1k 2-D carbon fiber.  The patterned area typically ranges from 7-10 cm^2, depending on the type of mold and if defects were present on the edges of the sample that were removed.  The size discrepancy of the molds, particularly between orthogonal and parallel samples arises from limitations of the CD or DVD disk size in the radial direction.  The edges are trimmed off in order to eliminate edge effects that arise when resin wicks over the mold.    The bottom of the samples are not this messy or frayed when they are tested, this is a result of pulling the fabric off of a layer of scotch tape that is used to hold the sample down in the clamp.


 

Monday, April 23, 2012

Patterned Adhesion with Composites

In these experiments, 5 composites were made with 2-D (orthotropic) carbon fibers (1k) and F-15 polyurethane resin.  One sample was left unpatterned as a control sample to compare how features effect adhesion.  Two samples were created with a CD pattern, one with the lines running parallel to the straining direction and one orthogonal to the straining direction.  This was also repeated with a DVD pattern to compare two different size pitches.  The adhesion results are posted below with the adhesion in N/cm2 and the second graph is the normalized adhesion compared to the unpatterned surface.  All of these samples were tested for their adhesion on three different surfaces: Smooth glass, Frosted Glass and Painted Steel to evaluate the effect of different surface roughness on the adhesion.


The patterns with the CD features appear to do better than smooth samples in all three surfaces.  DVD patterns did better in the smooth adhesion, but not in the roughness.  One possibility is that since these features are smaller than the roughness, it may have a hard time fitting in and thus compromising the ability to adhere.  In the CD the patterns are closer to the size of the roughness, and thus may be able to accommodate roughness better in the trenches.  More tests will follow on other substrates, it took a few attempts to get a fairly consistent replicating method.