Monday, March 28, 2011

Dry CO2 exposure in Glovebag and Adhesion


Here is a force vs. displacement curve for two glass surfaces treated with a 21 hour vapor exposure of N-(2-ethylamino)-3-aminopropyl trimethoxysilane. One of the surfaces was left untreated, the second one was left in a glove bag for 2 hours under a dry N2 gas purge. Following the purge, the sample was exposed to a 90 second exposure to "Bone Dry" Grade CO2 in the same glove bag. The sample exposed to CO2 showed very little change in contact angle measurements. Here is the force vs. displacement curve for the two samples and little differences were exhibited in the adhesion.

Monday, January 31, 2011

Submerged Adhesion of Amino Functionalize Surfaces

In this picture, this is a force vs. displacement for a PDMS probe on non-functionalized glass (red), amine functionalized glass (N-ethylamino-3proplyaminetrimethoxysilane, in blue), and the same silane treatement with CO2 exposure (in green). The probe speed was 1 micron/sec. Subsequent trials of this adhesion test will follow shortly.

Wednesday, December 8, 2010

Compression Testing of Amine Layers

In this sequence of microscope images (2.5 x magnification), a glass probe was compressed against glass slide samples that were prepared on 10-12-2010 with N-(2-aminoethyl)-3-aminopropyl-trimethoxysilane as the layer. The top image is that of the probe coming into contact with a large droplet and compressing down to 1 g of force on a glass slide that has had CO2 added to it. The second droplet is another image of the same slide, however this time the compression test was done on an area that did not have a large droplet. The third image is that of the same silane treatment, but a sample that has not had any CO2 added at all. The scale bar for all three images is 500 microns and all of these images are at the point of maximum force applied.




Monday, October 18, 2010

Drying Effects

More on the contact angles will be posted when I compile a couple of more samples, but for now here are some images of the effects of drying the samples with CO2 gas versus air when wet with water. The samples were prepared by vapor deposition, similar to the procedure used in prior blog postings. The pictures are: Amine surface [N-(2-aminoethyl)-3-aminopropyl-trimethoxysilane] after drying with CO2 (top left), air dry (bottom left), formamidine functionalized with CO2 drying (top right) and formamidine functionalized with air drying (bottom right). The magnification of these pictures is 5x ( I apologize for no scale bars).







Thursday, October 7, 2010

More contact angle measurements

Continuing from the last post, here are the contact angles of the converted amine surfaces to amidine surfaces:

With CO2 in water treatment for 5 minutes:
75.4 +/- 2.9 (Advancing)
32.0 +/- 3.4 (Receding)

With N2 in water treatment for 5 minutes:
80.6 +/- 2.2 (Advancing)
29.6 +/- 6.4 (Receding)

Tuesday, October 5, 2010

Amine Functionalized Slides Contact Angle Measurements

The initial contact angles of 3-aminopropyl-dimethyl ethoxysilane:

Slide 1: 73.8 +/- 1.9 (Advancing)
23.4 +/- 4.6 (Receding)

Slide 2: 73.6 +/- 2.8 (Advancing)
25.8+/- 2.9 (Receding)

This compares with 68.4 and 45.2 (advancing and receding respectively, Smith and Chen, Langmuir 2008, 24, 12405-12409)

Only variations to their procedure were UVO treatment opposed to Piranha etching and the post-cure step was done under vacuum rather than ambient atmosphere.

Two more samples prepared at the same time, that were reacted to form the formamidine analog, will be posted their contact angles, dry, with water/N2 and with water/CO2, will be posted tomorrow.

Monday, September 20, 2010

Amidne Glass Surface Roughness

Images shown below are AFM images of formamidine functionalized glass. The top two are two separate examples of when samples were submerged and N2 gas was bubbled in. The bottom two are examples of when CO2 is bubbled in. All of the areas are 3x3 um and the scan rate is 1 Hz. The height ranges from 0-25 nm.